Technical | Analysis of common injection molding defects and solutions

Author: ComeFrom: Date:2022/1/19 11:05:40 Hits:587
Technical | Analysis of common injection molding defects and solutions
发布时间:2019/5/28 17:07:50 点击次数:1370

Technical | Analysis of common injection molding defects and solutions

To do plastic, you need to supplement some knowledge of plastic molds, and now Xiaobian shares with you the analysis and countermeasures of the causes of plastic injection molding defects


一、Burr problems




Undesirable phenomenon: When we see that there is a flying edge on the edge of the figure below, do not rush to conclusions;

Solutions: It can be analyzed from the following three aspects:

1: The clamping force is too small; 2: The mold gap is too large; 3: Analyze the molding conditions: temperature, pressure, time, speed, metering;

二、Stress marks


Stress marks are due to the presence of obvious changes in thickness in the original design of the assembly, resulting in deformed stress trace defects in the finished plastic parts. Usually the stress marks will be more obvious on the back of the finished plastic part.

Solutions:

1: Pay attention to the consistency of meat thickness when structural design, and there can be no mutation of meat thickness;

2: Mold to strengthen cooling, such as increasing waterways;


三、Dents/sink marks


Undesirable phenomenon: Dents refer to the depressions formed on the local surface of the plastic parts in places where the plastic flesh is thick such as ribs, ribs, and inner insert areas. Thick areas of meat are not adequately compensated by plastic when cooled.

Solutions:

1: The glue reduction treatment can be carried out in the place of glue thickness to reduce the risk of shrinkage;

2: Appropriately increase the pressure holding and replenishment;

3: Strengthen waterway cooling.


四、Weld wires


Undesirable phenomenon: The welding wire is produced by the fusion glue in the filling process, because the flow wavefront of more than two directions is brought together, and the weld line affects the appearance problem, which will lead to the strength of the structural parts when it is serious.

Solutions: 1: Change the gate position 2: Gradient wall thickness 3: Needle valve gate sequence control


五、char


Undesirable phenomena: The following figure on the right has poor injection burn, which is caused by injection molding sleepy gas;

Solution: Add exhaust gas on the sub-mold surface, the location is as follows




六、Flow marks


Undesirable phenomenon: Flow marks are defects in which the plastic part creates water waves on the surface near the gate. This defect usually occurs when the gate is set in the middle of the cavity

Solution: You can simulate injection molding through mold flow analysis, select the best runner, and modify the injection pressure curve to solve the problem of flow pattern


七、Short shots


Undesirable phenomenon: Short shot is due to the fact that after completing the production process, the melt glue still cannot completely fill the mold cavity, resulting in a defective appearance of the final plastic part. Short shots are most likely to occur in thin areas or at the end of the flow.

Solutions:

1: The structural design pays attention to the control of meat thickness, and it is recommended that the thinnest meat thickness is not less than 0.5mm;

2: Replace the injection molding machine with a large injection volume;

3: Increase screw forward time.


八、Gate print


Undesirable phenomenon: appears on the back of the submerged gate or horn gate, caused by a large shear rate at the inlet gate

Solution: Without affecting the assembly, add a rubber nozzle convex bag at the inlet and outlet, and the thickness of the raised glue is about 0.2 thickness.

The above is a common injection molding defect analysis, as an engineer to deal with the problem of injection molding, generally look, smell, ask, cut four steps, from the table and inside the comprehensive analysis, catch the main cause before taking effective solutions


Recommended reading:



Next:The black technology that saved the next
unshan Gu'an Automation Machinery Co., Ltd

Business hotline: Miss Liu 13776319563

Technical support: Gu Gong 18913224469

e-mail address:gooaon@163.com

Ali Wangpu:https://www.gooaon.com.cn

Address: No. 56, Gangpu East Road, Zhangpu Town, Kunshan City, Suzhou, Jiangsu Province

Product selection

technical support

Copyright © 版权所有:Kunshan Gu'an Automation Machinery Co., Ltd. 备案号:苏ICP备13050163号 技术支持:拾久科技